Causes of Bolt Fracture in Valve Flange Connections
On this page

Abstract

A bolt in a valve flange connection at a petroleum refining and petrochemical plant fractured during service. To identify the cause of failure, a comprehensive investigation was conducted using a Zeiss scanning electron microscope (SEM), a direct-reading spectrometer, a hardness tester, and a metallographic microscope. The results revealed the following:

Fracture morphology: The fracture surface exhibited a characteristic rock-candy-like intergranular morphology. Analysis of the corrosion products confirmed the presence of chlorine (Cl).

Metallographic examination: The grain boundaries were coarsened, resulting in reduced intergranular cohesion.

Chemical composition: The carbon (C) content was excessively high, while the chromium (Cr) and nickel (Ni) contents were relatively low.

Hardness testing: The bolt hardness exceeded the specified limits.

These findings indicate that the bolt fracture was primarily caused by improper solution heat treatment and an unsuitable chemical composition. Inadequate solution heat treatment resulted in grain boundary coarsening and reduced intergranular cohesion. In addition, the improper heat treatment, combined with the high carbon content, contributed to abnormally high hardness. In the chlorine-containing service environment, the low chromium and nickel contents impaired the corrosion resistance of the stainless steel. Chloride ions (Cl⁻) penetrated the passive film, accelerating corrosion of the underlying material and ultimately leading to brittle fracture.

 

Introduction

Petroleum is a major primary energy source and is widely used in various sectors, including industry, the military, and agriculture, where it plays an important role in economic and social development. However, naturally occurring petroleum that can be used directly without refining is extremely limited. Most crude oil must therefore undergo refining to produce usable petroleum products. Consequently, the safe and reliable operation of refining and petrochemical equipment is essential to ensuring a stable supply of petroleum products and safeguarding national energy security. During a routine inspection at a petrochemical refinery, a leak was discovered at a valve flange connection. The inspection team promptly shut off the main valve, necessitating an unplanned shutdown of the entire production line. After the flange connection was disassembled, a fractured bolt was found. To identify the cause of the failure and prevent similar incidents, a systematic failure analysis was conducted.

 

1 Physical and Chemical Testing and Results

1.1 Macroscopic Examination

The fractured bolt is shown in Figure 1. As shown, the bolt exhibits two secondary fracture surfaces. It is inferred that the initial fracture went undetected during inspection, allowing secondary fractures to develop under subsequent cyclic loading. In addition, yellowish-brown corrosion products, likely oxides, were observed on the bolt surface. Similar products were also present on the fracture surfaces. This suggests that the fractured bolt was not removed promptly after the initial failure, leaving the newly exposed fracture surfaces in contact with moisture and oxygen in the surrounding environment. The resulting conditions promoted corrosion at the fracture sites.

Macroscopic Appearance of the Fractured Bolt

(a) Front View (b) Top View

Figure 1. Macroscopic Appearance of the Fractured Bolt

 

1.2 Chemical Composition Analysis

The chemical composition of the failed bolt was analyzed using an OBLF direct-reading spectrometer manufactured in Germany. Because of the bolt's cylindrical geometry, direct measurements on its outer surface could introduce errors. Therefore, a section was cut from the failed bolt and used as the test specimen, with measurements performed on the cut end face, as shown in Figure 2.

Location of Chemical Composition Analysis on the Bolt

Figure 2. Location of Chemical Composition Analysis on the Bolt

 

The analysis results showed that the bolt material consisted primarily of C, Si, Mn, P, S, Cr, Mo, Ni, and Fe. Comparison with GB/T 20878-2024, Stainless Steels—Grades and Chemical Composition, revealed that the carbon (C) content exceeded the specified limit, while the chromium (Cr) and nickel (Ni) contents, although within the standard's specified ranges, were relatively low. The chemical composition of the bolt is presented in Table 1. In general, increasing the carbon content enhances material strength. However, excessive carbon increases hardness and reduces toughness, thereby increasing the risk of brittle fracture.

 

1.3 Hardness Testing

Hardness is a measure of a material's resistance to localized deformation, indentation, and scratching, and is an important mechanical property. To evaluate the hardness of the failed bolt, hardness testing was performed at three points along the radial direction of the specimen. The average value was then calculated and compared with the requirements of GB/T 20878-2024. The test results are presented in Table 2.

 

Table 1. Chemical Composition of the Bolt (Mass Fraction, %)

Element

C

Si

Mn

P

S

Cr

Mo

Ni

Measured value

0.100

0.590

0.932

0.033

0.027

18.310

0.843

8.080

Standard requirement

≤0.070

≤1.000

≤2.000

≤0.035

≤0.030

18.000–20.000

0.800–1.300

8.000–11.000

 

Table 2. Hardness Test Results for the Bolt

Measurement Point

Measured Hardness (HV)

Standard Limit (HV)

1

310.0

≤220

2

330.0

≤220

3

342.0

≤220

Average

327.3

≤220

 

As shown in Table 2, the hardness values at all three measurement points exceeded the specified limit. In general, increasing the carbon (C) content tends to increase both the hardness and strength of a material. However, excessive carbon content can lead to excessively high hardness and reduced toughness, thereby increasing the susceptibility to brittle fracture.

 

1.4 Metallographic Examination

To determine whether the bolt material exhibited any microstructural abnormalities, its microstructure was examined using a metallographic microscope, as shown in Figure 3. The micrograph reveals distinct annealing twins, indicating that the failed bolt is made of austenitic stainless steel. Further examination revealed that the grains were coarser than those typically observed in austenitic stainless steel. In general, grain coarsening reduces the total grain boundary area and the resistance to dislocation motion, which would theoretically result in lower material hardness. However, the failed bolt exhibited abnormally high hardness, suggesting that work hardening may have occurred during manufacturing processes such as cold heading or machining. Solution heat treatment is generally required to eliminate work hardening. Inadequate solution heat treatment may result in excessive hardness and grain boundary degradation. Grain coarsening also reduces intergranular cohesion, making the material more susceptible to crack initiation and subsequent fracture under mechanical loading.

Metallographic Microstructure of the Bolt (1,000× Magnification)

Figure 3. Metallographic Microstructure of the Bolt (1,000× Magnification)

 

2 Microscopic Examination of the Fracture Surface

2.1 SEM Examination of the Fracture Surface

Identifying the failure mode is essential to determining the root cause of material failure. In this study, the fracture surface of the failed valve bolt was examined using a Carl Zeiss scanning electron microscope (SEM, Germany). Because the bolt was not removed immediately after fracture, substantial contamination had accumulated on the fracture surface, severely hindering microscopic observation. To improve image clarity, the fracture surface was cleaned in an ultrasonic cleaner for 10 min before being re-examined by SEM. The results are shown in Figure 4.

SEM Image of the Bolt Fracture Surface (800× Magnification)

Figure 4. SEM Image of the Bolt Fracture Surface (800× Magnification)

 

As shown in Figure 4, the fracture surface exhibits a characteristic rock-candy-like morphology, indicating intergranular cracking, a form of brittle fracture. This suggests that the bolt was susceptible to brittle fracture under service loading, potentially due to its excessively high hardness.

 

2.2 Corrosion Product Analysis

The bolt was used in a petrochemical facility, where it was exposed to a relatively harsh operating environment. To determine whether corrosion contributed to the failure, the corrosion products on the bolt fracture surface were analyzed. Since the bolt was not properly preserved after fracture, contaminants had accumulated on its surface. The fracture surface was therefore cleaned before analysis. The results are presented in Figure 5.

Analysis of Corrosion Products on the Bolt Fracture Surface

Figure 5. Analysis of Corrosion Products on the Bolt Fracture Surface

 

As shown in Figure 5, the fracture surface contains Cr, Ni, Fe, O, and Cl. Fe, Cr, and Ni are constituent elements of the bolt material, whereas Cl is a major contributor to stainless steel corrosion and is strictly controlled during stainless steel production. Therefore, the chlorine detected on the fracture surface was likely introduced from an external source rather than being inherent to the material. An on-site inspection revealed that the plant is located only a few hundred meters from the coastline. Humid sea breezes may therefore have carried seawater into the plant area, exposing the bolts to chloride ions (Cl⁻), which can damage the passive film and accelerate corrosion of the stainless steel. Under alternating service stresses, the corrosion-damaged bolts eventually fractured.

 

3 Failure Cause Analysis

Chemical composition analysis revealed an excessively high carbon (C) content and chromium (Cr) and nickel (Ni) contents at the lower ends of their specified ranges. Although carbon can increase material strength, excessive carbon content may lead to increased hardness and reduced toughness, making the material more susceptible to brittle fracture. The relatively low Cr and Ni contents also impair the corrosion resistance of the stainless steel. Hardness testing confirmed that the bolt hardness exceeded the specified limit, further increasing its susceptibility to brittle fracture under service loading. Metallographic examination revealed coarse grains, suggesting that improper solution heat treatment may have contributed to the abnormal microstructure and reduced intergranular cohesion. SEM examination confirmed an intergranular brittle fracture morphology, while energy-dispersive X-ray spectroscopy (EDS) detected chlorine (Cl) on the fracture surface. Austenitic stainless steel normally exhibits good corrosion resistance because a protective passive film forms on its surface, separating the underlying metal from the surrounding environment. However, chloride ions (Cl⁻) can locally break down this passive film, initiating corrosion and accelerating material degradation. Under the combined effects of chloride-induced corrosion and alternating service stresses, the bolt ultimately fractured.

 

4 Conclusion

Chemical composition analysis revealed an excessively high carbon (C) content and relatively low chromium (Cr) and nickel (Ni) contents, which increased the susceptibility to brittle fracture and impaired corrosion resistance. Hardness testing confirmed that the bolt hardness exceeded the specified limit, while metallographic examination revealed coarse grains and reduced intergranular cohesion. SEM examination identified intergranular brittle fracture, and EDS detected chlorine (Cl) on the fracture surface, indicating that corrosion contributed to the failure. Overall, the abnormal chemical composition and improper post-fabrication solution heat treatment resulted in excessive hardness and reduced resistance to intergranular fracture. Combined with the corrosive service environment and alternating stresses, these factors ultimately led to bolt fracture.


To prevent similar incidents from recurring, the following measures are recommended:

(1) Strengthen material inspection before bolt installation to ensure that nonconforming bolts are not put into service.

(2) Enhance routine inspections. If any equipment abnormality is detected, promptly shut down the system and investigate the cause to prevent accidents.

(3) Given the high chloride ion (Cl⁻) concentration in the bolt's service environment, implement appropriate corrosion protection measures after installation or replace the bolts with materials offering better corrosion resistance to prevent recurrence of similar failures.